Hardness Conversion Chart: HRC, HRB, HV, HB (ASTM E140)
Hardness scales measure different things (indentation depth for Rockwell, indentation area for Vickers and Brinell), so there is no exact formula between them. For steel, ASTM E140 gives empirical equivalents: 40 HRC ≈ 392 HV ≈ 371 HBW ≈ 70.4 HRA. Every converted number is approximate and only valid for the material group the table was made for.
Size chartSort by any column, or filter to find a row
| Rockwell | HVVickers HV | HBWBrinell HBW 10/3000 | HRARockwell A (HRA) | HR15NSuperficial HR15N | HR30NSuperficial HR30N | HR45NSuperficial HR45N | HR15TSuperficial HR15T | Tensile strength ≈ (ISO 18265)MPaksi |
|---|---|---|---|---|---|---|---|---|
| Rockwell C range (HRC 68–20), ASTM E140 Table 1 | ||||||||
| 68 HRC | 940 | — | 85.6 | 93.2 | 84.4 | 75.4 | — | — |
| 67 HRC | 900 | — | 85.0 | 92.9 | 83.6 | 74.2 | — | — |
| 66 HRC | 865 | — | 84.5 | 92.5 | 82.8 | 73.3 | — | — |
| 65 HRC | 832 | — | 83.9 | 92.2 | 81.9 | 72.0 | — | — |
| 64 HRC | 800 | — | 83.4 | 91.8 | 81.1 | 71.0 | — | — |
| 63 HRC | 772 | — | 82.8 | 91.4 | 80.1 | 69.9 | — | — |
| 62 HRC | 746 | — | 82.3 | 91.1 | 79.3 | 68.8 | — | — |
| 61 HRC | 720 | — | 81.8 | 90.7 | 78.4 | 67.7 | — | — |
| 60 HRC | 697 | — | 81.2 | 90.2 | 77.5 | 66.6 | — | — |
| 59 HRC | 674 | 634 | 80.7 | 89.8 | 76.6 | 65.5 | — | — |
| 58 HRC | 653 | 615 | 80.1 | 89.3 | 75.7 | 64.3 | — | — |
| 57 HRC | 633 | 595 | 79.6 | 88.9 | 74.8 | 63.2 | — | 2115307 |
| 56 HRC | 613 | 577 | 79.0 | 88.3 | 73.9 | 62.0 | — | 2040296 |
| 55 HRC | 595 | 560 | 78.5 | 87.9 | 73.0 | 60.9 | — | 1975286 |
| 54 HRC | 577 | 543 | 78.0 | 87.4 | 72.0 | 59.8 | — | 1910277 |
| 53 HRC | 560 | 525 | 77.4 | 86.9 | 71.2 | 58.6 | — | 1845268 |
| 52 HRC | 544 | 512 | 76.8 | 86.4 | 70.2 | 57.4 | — | 1790260 |
| 51 HRC | 528 | 496 | 76.3 | 85.9 | 69.4 | 56.1 | — | 1730251 |
| 50 HRC | 513 | 481 | 75.9 | 85.5 | 68.5 | 55.0 | — | 1675243 |
| 49 HRC | 498 | 469 | 75.2 | 85.0 | 67.6 | 53.8 | — | 1625236 |
| 48 HRC | 484 | 455 | 74.7 | 84.5 | 66.7 | 52.5 | — | 1570228 |
| 47 HRC | 471 | 443 | 74.1 | 83.9 | 65.8 | 51.4 | — | 1525221 |
| 46 HRC | 458 | 432 | 73.6 | 83.5 | 64.8 | 50.3 | — | 1480215 |
| 45 HRC | 446 | 421 | 73.1 | 83.0 | 64.0 | 49.0 | — | 1440209 |
| 44 HRC | 434 | 409 | 72.5 | 82.5 | 63.1 | 47.8 | — | 1400203 |
| 43 HRC | 423 | 400 | 72.0 | 82.0 | 62.2 | 46.7 | — | 1360197 |
| 42 HRC | 412 | 390 | 71.5 | 81.5 | 61.3 | 45.5 | — | 1325192 |
| 41 HRC | 402 | 381 | 70.9 | 80.9 | 60.4 | 44.3 | — | 1295188 |
| 40 HRC | 392 | 371 | 70.4 | 80.4 | 59.5 | 43.1 | — | 1260183 |
| 39 HRC | 382 | 362 | 69.9 | 79.9 | 58.6 | 41.9 | — | 1225178 |
| 38 HRC | 372 | 353 | 69.4 | 79.4 | 57.7 | 40.8 | — | 1195173 |
| 37 HRC | 363 | 344 | 68.9 | 78.8 | 56.8 | 39.6 | — | 1165169 |
| 36 HRC | 354 | 336 | 68.4 | 78.3 | 55.9 | 38.4 | — | 1135165 |
| 35 HRC | 345 | 327 | 67.9 | 77.7 | 55.0 | 37.2 | — | 1110161 |
| 34 HRC | 336 | 319 | 67.4 | 77.2 | 54.2 | 36.1 | — | 1080157 |
| 33 HRC | 327 | 311 | 66.8 | 76.6 | 53.3 | 34.9 | — | 1050152 |
| 32 HRC | 318 | 301 | 66.3 | 76.1 | 52.1 | 33.7 | — | 1025149 |
| 31 HRC | 310 | 294 | 65.8 | 75.6 | 51.3 | 32.5 | — | 995144 |
| 30 HRC | 302 | 286 | 65.3 | 75.0 | 50.4 | 31.3 | — | 970141 |
| 29 HRC | 294 | 279 | 64.6 | 74.5 | 49.5 | 30.1 | — | 945137 |
| 28 HRC | 286 | 271 | 64.3 | 73.9 | 48.6 | 28.9 | — | 920133 |
| 27 HRC | 279 | 264 | 63.8 | 73.3 | 47.7 | 27.8 | — | 895130 |
| 26 HRC | 272 | 258 | 63.3 | 72.8 | 46.8 | 26.7 | — | 870126 |
| 25 HRC | 266 | 253 | 62.8 | 72.2 | 45.9 | 25.5 | — | 855124 |
| 24 HRC | 260 | 247 | 62.4 | 71.6 | 45.0 | 24.3 | — | 835121 |
| 23 HRC | 254 | 243 | 62.0 | 71.0 | 44.0 | 23.1 | — | 815118 |
| 22 HRC | 248 | 237 | 61.5 | 70.5 | 43.2 | 22.0 | — | 795115 |
| 21 HRC | 243 | 231 | 61.0 | 69.9 | 42.3 | 20.7 | — | 780113 |
| 20 HRC | 238 | 226 | 60.5 | 69.4 | 41.5 | 19.6 | — | 765111 |
| Rockwell B range (HRB 100–80), ASTM E140 Table 2 | ||||||||
| 100 HRB | 240 | 240 | 61.5 | — | — | — | 93.1 | 770112 |
| 95 HRB | 210 | 210 | 58.3 | — | — | — | 91.5 | 67598 |
| 90 HRB | 185 | 185 | 55.2 | — | — | — | 89.9 | 59586 |
| 85 HRB | 165 | 165 | 52.3 | — | — | — | 88.2 | 53077 |
| 80 HRB | 150 | 150 | 49.5 | — | — | — | 86.6 | 48070 |
No exact match. The nearest sizes:
How to read a hardness value
A hardness value is written as the number first, then the scale: 58 HRC, 210 HV10, 280 HBW 10/3000. The suffix after HV or HBW is the test load (HV10 = 10 kgf; HBW 10/3000 = 10 mm tungsten carbide ball, 3000 kgf). A number without its scale means nothing: 60 HRB is soft annealed steel, 60 HRC is a file.
Rockwell C (diamond cone, 150 kgf) is the scale for hardened steel, roughly 20–70 HRC. Below 20 HRC it is not valid; use Rockwell B (1/16 in ball, 100 kgf), which covers soft steel and brass up to about 100 HRB. HRA (diamond cone, 60 kgf) is used for very hard materials such as cemented carbide and thin hard layers.
Superficial Rockwell scales (HR15N, HR30N, HR45N: diamond cone at 15, 30, 45 kgf) leave a shallow dent and are used on thin sheet, small parts and case-hardened surfaces. Vickers (diamond pyramid) works across the whole range and is the reference scale of ISO 18265. Brinell uses a 10 mm ball and a large load; it averages over coarse structures (castings, forgings) but is limited to about 650 HBW.
Rows in parentheses in the original E140 table, and all Brinell values above 650, are outside the range of the test method; we leave them blank instead of printing numbers nobody can measure. Where Table 1 and Table 2 meet they do not join exactly (100 HRB = 240 HV = 240 HB, while 20 HRC = 238 HV = 226 HBW), which shows how approximate the whole exercise is.
About Hardness Conversion
Use this table to compare a supplier's figure with your drawing, to check whether a heat treatment is plausible, or to pick a test method. Do not use it to accept parts: if the drawing calls for 58–62 HRC, the part must be tested in HRC. ASTM E140 and ISO 18265 both state that converted values are approximate and may not be used where the specification names a scale.
The rows apply to non-austenitic steels: carbon, alloy and tool steels in the annealed, normalised and quenched-and-tempered condition. Austenitic stainless steel, cold-worked metal, aluminium, copper alloys, cast iron and nickel alloys have their own tables in E140 because their work-hardening behaviour shifts the relation between scales.
Between rows, interpolate linearly; the calculator above does that for any scale. Report the converted value as an estimate, for example "≈ 390 HV (converted from 40 HRC, ASTM E140)".
The tensile strength column is a rough estimate from ISO 18265 Table A.1, which relates Vickers hardness to tensile strength for unalloyed and low-alloy steels. ISO 18265 itself calls the strength estimate the least reliable conversion in the standard; expect a scatter of ±10 % or more against a real tensile test, and do not use it for high-alloy, cold-worked or case-hardened material.
Typical hardness of common parts
Orientation values only. The actual range is set by the material standard or the drawing.
| Part / condition | Typical hardness |
|---|---|
| Mild steel S235, 1018 hot rolled | ≈ 120–160 HB (≈ 70–85 HRB) |
| 1045 / C45 normalised | ≈ 170–210 HB |
| 4140 / 42CrMo4 quenched and tempered (pre-hardened bar) | ≈ 28–32 HRC |
| Property class 8.8 bolt (ISO 898-1) | ≈ 22–34 HRC (250–335 HV) |
| Property class 12.9 bolt (ISO 898-1) | ≈ 39–44 HRC (385–435 HV) |
| Socket wrench, hand tools (Cr-V) | ≈ 40–50 HRC |
| Knife blade, stainless | ≈ 54–60 HRC |
| Ball bearing ring, 52100 / 100Cr6 | ≈ 58–65 HRC |
| File, HSS drill, D2 punch | ≈ 60–66 HRC |
Which test to choose
Minimum thickness: the part must be at least about 10 times the indentation depth (Rockwell) or 1.5 times the diagonal (Vickers) thick, or the anvil shows through. That is why thin sheet is tested with HR15N or HR30T, and case-hardened layers with Vickers HV1 or less across a cross-section.
Coarse or mixed structure (cast iron, forgings, welds over a large area): Brinell. Hardened tool steel: Rockwell C. Small parts, thin layers, weld heat-affected zones: Vickers. Field checks on large parts: portable rebound (Leeb) or UCI testers, which are themselves conversions and need calibration on similar material.
Questions
What is 40 HRC in Vickers and Brinell?
About 392 HV and 371 HBW (ASTM E140, steel). In the other direction, 400 HV is about 40.8 HRC.
How do I convert HRC to tensile strength?
Only approximately. For quenched-and-tempered carbon and low-alloy steel, ISO 18265 Table A.1 gives about 1260 MPa for 40 HRC (392 HV), about 970 MPa for 30 HRC (302 HV) and about 1675 MPa for 50 HRC (513 HV), interpolated between its rows. A tensile test is the only real value.
Is Brinell hardness the same as Vickers?
Close below about 250: in the soft range of E140 Table 2 the HB (3000 kgf) and HV numbers are identical (e.g. 90 HRB = 185 HV = 185 HB). Above that Brinell reads lower, because the ball flattens: 50 HRC is 513 HV but 481 HBW.
What is 100 HRB in HRC?
100 HRB is about 240 HV, which sits just above 20 HRC (238 HV). The two Rockwell scales only overlap around this point; HRC below 20 and HRB above 100 are outside the valid range of each test.
Why does my HRC to HV conversion differ between charts?
Charts are based on different standards (ASTM E140, ISO 18265, SAE J417, older DIN 50150) and material groups. Differences of 1 HRC or 10 HV are normal; the conversion itself is no more precise than that.
Sources
- ASTM E140-12b(2019)e1: Standard Hardness Conversion Tables for Metals (Tables 1 and 2, non-austenitic steels)
- ISO 18265:2013, Metallic materials, Conversion of hardness values (Table A.1, unalloyed and low-alloy steels)
- SAE J417: Hardness tests and hardness number conversions (as reproduced by Misumi)
- Mitutoyo: Hardness conversion chart (based on ASTM E140)
- WS-Stahl: Steel hardness comparison table to DIN EN ISO 18265 Table A.1
- Portland Bolt: Steel hardness conversion chart (Brinell 3000 kgf, Rockwell B and C)
Values last checked against these sources on November 15, 2026. · How we check data
Reference values for planning and identification. Confirm critical dimensions with the manufacturer's drawing or the current edition of the standard before production.